Centrifugal vs Static PU Casting: Choosing a Liner Method Banner background

Centrifugal vs Static PU Casting: Choosing a Liner Method

Choosing between centrifugal and static PU casting for hollow liners comes down to what holds the wall in place. In centrifugal casting the mold spins...

Choosing between centrifugal and static PU casting for hollow liners comes down to what holds the wall in place. In centrifugal casting the mold spins and the resin is thrown outward against the bore, so no core is needed, and wall thickness is set by shot mass, spin speed and gel time. In static casting the resin fills the annulus between a core and an outer mold, so wall thickness is set by core concentricity, venting and pour rate. Most liner problems trace back to whichever of those two variable sets the chosen method makes harder to control, which is why the decision should follow the part geometry rather than the machine catalogue.

How Each Method Builds the Liner Wall

A centrifugal liner is cast in a tubular mold mounted on a spindle. The shot enters at one end of the spinning mold and is driven outward, so the inner surface of the part is formed by the resin itself while air is displaced toward the axis and escapes through the open end or a vent. Because no core defines the inside diameter, the finished wall is the result of the volume you fed divided by the bore area. Feed a light shot and the wall thins uniformly; feed a heavy shot and the excess has to go somewhere, usually into the end trim or a heavier section near the pour point.

Compaction pressure at the bore wall rises with the square of rotational speed and with the difference between outer and inner radius. That relationship explains both the benefit and the cost of spinning. Enough speed wets the mold surface and pushes air inward; much more speed mainly increases the force that separates fillers by density and loads the spindle bearings.

a47

Static casting reverses the geometry. A core sits inside the mold, the annulus between them is the part, and the resin is poured into a cavity whose dimensions are already fixed by tooling. The pour has to push air ahead of it through a narrow gap, so vent placement and pour rate matter more than shot volume once the cavity is full. Wall thickness error therefore comes from the core, not from the metering pump: core deflection along a long span, core position at each end, and clamping distortion all show up directly in the liner section. Static casting also cures with the part restrained on both faces, which changes where shrinkage appears compared with a free inner surface.

Where Each Method Fails First

Centrifugal liners tend to fail in the axial direction. If gel time is shorter than the time needed to distribute resin from the feed end to the far end, the part tapers before the resin reaches the tip. Spindle runout and bearing wear print themselves as a wall that is thin at one clock position along the whole length. Dense fillers move outward, leaving a resin-rich inner layer and a filler-rich outer layer. Air that cannot travel to the open end stays as small bubbles just under the inner surface.

Static liners fail at the fill end and around the core. Air pockets collect under flanges and at the top of the annulus. A long unsupported core bows under pour pressure, so the wall is thin on one side and thick on the opposite side at mid-length. Slow pouring into a cold mold produces cold joints and visible knit lines. Thick sections sink because the core and mold hold the surfaces while the interior contracts.

These locations are well established from the mechanics of each process. Which cause is active in a specific plant still has to be confirmed by sectioning a part, weighing shots and dial-testing tooling, not assumed from a defect name.

Symptom Typical location Method most exposed First check
Wall varies around the bore one clock position, full length Centrifugal dial-test the spinning mold and spindle runout
Air pockets under a flange upper fill end Static vent location and end-of-fill pour rate
Filler concentrated outward outer third of the wall Centrifugal filler density against resin, spin speed profile
Axial taper toward the far end opposite the pour point Centrifugal gel time against distribution time
Sink or internal void in a thick section thickest wall, hot spot Static shot mass, mold temperature, cure schedule

a48

Metering, Shot Weight and Spin Speed

Start with the volume of the wall: π/4 × (OD² − ID²) × L, multiplied by the mixed density of the system, with an allowance for runners and end trim. In a centrifugal liner that number is the thickness control. In a static liner the same number only decides whether the cavity fills; the core decides the wall.

Shot mass error has nowhere to go in a centrifugal liner, because the bore is formed by the resin surface rather than a core. <How To Calculate Shot Weight In Polyurethane> covers how shot weight is calculated for polyurethane parts.

That difference changes what you buy. A centrifugal cell needs feed accuracy and spin synchronization more than it needs a large tank: the shot is small relative to the mold, and a small error is a direct thickness error. A static cell needs enough pour rate to fill the annulus before gel and enough vacuum to strip dissolved air out of a viscous prepolymer before it enters a narrow gap. On the casting units used for pipe lining work, such as the HF-CPUE-2A2B-PipeLiner, the published figures are a 100 to 1500 g/s pour rate, ±0.3% full-range dosing accuracy, MOCA ratios of 100:10 to 100:13 and BDO ratios of 100:4 to 100:6, with vacuum defoaming at −0.095 MPa or better. Those are machine capabilities, not a guarantee about the liner that comes out of the mold.

Spin speed has no universal setting. Size it from the bore radius and the compaction the resin needs, then check whether the extra speed is doing anything useful. Above the point where the wall is wetted and air has migrated inward, additional speed mostly increases filler separation and machine wear.

Core, Mold and Demolding Differences

Static tooling carries the cost that centrifugal tooling avoids. The core sets the inside diameter, so it needs draft, a surface finish that releases a tacky elastomer, and often internal heating to keep the resin from chilling against it. Long cores need support or tensioning to stay straight under pour pressure. Extraction direction has to be settled before the mold is built, because a liner with an internal step will not come off a one-piece core.

Rotational casting and mandrel casting share the same cure logic, so core preparation and demold timing affect surface quality as much as the pour does. <How Polyurethane Rollers Are Made From Casting To Cure> covers the casting-to-cure sequence for cast PU parts.

Centrifugal tooling avoids the core but pays elsewhere. The mold has to be balanced well enough to spin without whipping, the end closures have to seal without trapping air, and a long tube has to be extracted axially from a bore that has shrunk onto it. Even heating around the tube matters more than in static casting, because an uneven mold wall changes the gel front as the mold turns.

a77

When Centrifugal Casting Is the Right Choice

Centrifugal casting earns its place on long, slender, unfilled or lightly filled liners where a core would be the weakest element in the tooling. It also suits a product mix of few, long parts, because fill is fast and the mold is simple. It stops earning its place as soon as the part needs an internal feature, a closed end, a bonded insert, or a heavily filled abrasion grade.

Decision factor Centrifugal fits when Static fits when Do not choose centrifugal when
Length-to-bore ratio long slender tubes where a core would sag short, large-bore liners the mold cannot be spun without whipping
Wall tolerance tolerance achievable from shot mass control tolerance set by a machined core required tolerance is tighter than feed accuracy can hold
Filler content unfilled or density-matched fillers abrasive or heavy fillers the filler separates under acceleration
End geometry open ends or removable end caps closed ends, flanges, internal steps the part has a closed end or internal ribs
Inserts and bonding insert can be spun with the mold liner bonded to a steel shell the liner must bond to a fixed metal insert
Output model one long part per cycle with fast fill several small parts per cycle changeover frequency is high and molds are many

The two methods also differ in how a specification should be written. A centrifugal liner drawing should control wall thickness, mass per part and inner surface condition, because those are the variables the process can hold. A static liner drawing can control the inside diameter directly, so it should carry the core tolerance, the concentricity callout and the release requirements that make that tolerance real.

What the Records Do and Do Not Prove

Supplier case records are useful, but only for the specific claim they support. The table below separates what each record legitimately shows from the generalization a buyer should not draw.

Record Method context Responsible use Do not infer
E-bike tire centrifugal casting line, Jiangxi, full-servo units with ±2 g feed and casting-centrifuge linkage spinning mold, small parts, high volume feed accuracy and spin synchronization can be controlled to grams in a spinning-mold process that a liner mold will hold the same wall tolerance or reach the same yield
Rail pad rotary line, Hebei, patented precision pouring nozzle ZL 201611168678.6 static pour into closed molds, solid parts a fixed precision nozzle with multi-station indexing gives repeatable shots anything about concentricity of a hollow part, because the pad is solid
Pipe lining casting unit specification, 100 to 1500 g/s, ±0.3%, vacuum −0.095 MPa machine data sheet, not a production result what the equipment can deliver at the nozzle and in the vacuum chamber the quality of a finished liner without the mold, core and process
Rail pad automation project, Xi’an, parameters logged every five seconds turnkey line with full traceability every shot can be recorded and traced to a part dimensional capability of a different product or tooling set

What none of these records provide is a liner-specific acceptance number. That has to come from your own trial, measured on your own mold.

What to Verify in a Trial Before You Commit

  1. Fix the measurement plan before the first shot: wall thickness at three axial stations and four clock positions on every part, with eccentricity recorded as the maximum minus the minimum at each station.
  2. Section one part per condition. Look for voids, filler banding, knit lines, and the bond line if the liner sits on a steel shell.
  3. Weigh the shot rather than trusting the setpoint. In centrifugal casting that deviation is a thickness deviation; in static casting it is a short-fill risk.
  4. Time the gel against the fill and distribution time with a clock, not with a datasheet figure alone.
  5. Run long enough for mold temperature to stabilize, then keep running through a full demold and trim cycle, because extraction problems appear after the process looks stable.
  6. Agree acceptance criteria with the buyer before the trial starts: wall tolerance, surface condition, hardness on the agreed scale, and bond strength where relevant.

Hardness is the acceptance measurement most buyers write into the liner drawing, and it is read on a scale that differs from rigid plastic. <Shore A Vs Shore D Hardness In Polyurethane> covers the two hardness scales used for polyurethane.

a51

Specify the Liner and We Will Match the Method

Send the liner outside diameter, inside diameter, length, wall thickness tolerance, end geometry, and whether the part carries an insert or a flange. Add the PU system, MOCA or BDO, filler type and loading, target hardness, shot weight per part, cycle target, mold and core material, and whether the cell can spin a mold or must fill a closed annulus. With those inputs, the choice between centrifugal and static PU casting is a calculation rather than a preference, and the trial plan can be written before any tooling is cut.

Haifeng Polyurethane Machinery builds both casting and lining equipment, so the recommendation does not depend on selling one method. Contact us at Info@chinahaifeng.com or WhatsApp 86 13566296633 with the part drawing and the process data above.

FAQ

Can centrifugal casting produce a liner with a closed end?

Not in a simple tubular mold. A closed end traps air at the axis and blocks axial extraction of the finished part. Practical options are to cast the tube open-ended and bond a separately molded end cap, to use a split mold with a removable end former and a vent at the center, or to move the part to static casting where the cavity can be vented at its highest point. Each option adds a joint or a tooling cost, so it should be decided at the drawing stage.

Which method holds wall thickness better on a long liner?

It depends on length relative to bore. On a long slender liner, a core has to span the full part and stay straight under pour pressure, which is difficult, so centrifugal casting is usually more consistent because the wall is set by shot mass against a rigid spinning mold. On a short, large-bore liner the core is stiff and machined, and static casting is typically the more predictable route. Measure both options against your tolerance rather than choosing by habit.

Does filler in the PU change the choice?

Yes. Dense mineral fillers migrate outward under centrifugal acceleration, so the outer wall becomes filler-rich and the inner surface resin-rich. For an abrasion-resistant liner that gradient may be acceptable and even useful, but it has to be verified by sectioning rather than assumed. Heavily filled or density-mismatched systems are usually safer in static casting, where gravity-driven separation is slower and the pour can be kept short.

What shot weight accuracy do I need for a liner?

Work it back from the thickness tolerance. Multiply the allowed wall variation by the bore area and the mixed density to get an allowable mass error, then compare that with the machine’s dosing accuracy over the shot size you will actually run. A percentage figure alone tells you little, because the same ±0.3% is a small mass on a short part and a large one on a long liner. Weigh shots during the trial to confirm the real spread.

If you’re interested, check out these related articles:

How Polyurethane Rollers Are Made From Casting To Cure
The Role Of Rise Time In Polyurethane Foaming
What Is Spray Polyurethane Foam Composition And Application
SRIM Explained Structural Reaction Injection Molding Basics

Discuss Your Polyurethane Production Requirements

Share your application, material system, target output and automation requirements. Haifeng's engineering team can help you review equipment and production-line options. Our team will reply within one business day. Once requirements are clear, we provide a preliminary proposal within two business days.

Haifeng Polyurethane Machinery on TikTok
Haifeng Polyurethane Machinery on Instagram
Haifeng Polyurethane Machinery on Facebook
Haifeng Polyurethane Machinery on X
Haifeng Polyurethane Machinery on LinkedIn
Contact Haifeng Polyurethane Machinery on WhatsApp
Haifeng Polyurethane Machinery on YouTube